I had wanted to hold some of the good stuff for a future article, but realized there is a LONG way to go for a reasonably complete summary SO I went ahead and added what I have here
https://docs.google.com/document/d/1...EK8OtPYVA/edit

Scroll down to the bottom for the short version summary

Many thanks to Dave Suponski, Ron Graham, Raimey Ellenburg and Walt Snyder for their contributions, and Adam W. Haskins, P. E., Metallurgist at Metals Engineering and Testing Laboratories, METL in Phoenix, Arizona.

Last edited by Drew Hause; 02-24-2016 at 06:06 PM..
Drew Hause is offline   Reply With Quote
Visit Drew Hause's homepage!
Unread 02-25-2016, 11:11 AM   #2
Member
Bruce Day
PGCA Lifetime
Member
 
Bruce Day's Avatar

Member Info
 
Join Date: Nov 2008
Posts: 4,995
Thanks: 554
Thanked 15,664 Times in 2,672 Posts

Default

Drew, thank you for compiling and presenting this research. I have printed a copy and will refer this paper to others. Facts beat opinions any day to those who read and learn.
Bruce Day is offline   Reply With Quote
The Following 4 Users Say Thank You to Bruce Day For Your Post:
Unread 02-25-2016, 11:42 AM   #3
Member
Drew Hause
Forum Associate
 
Drew Hause's Avatar

Member Info
 
Join Date: Nov 2008
Posts: 2,177
Thanks: 341
Thanked 3,998 Times in 1,309 Posts

Default

It's been a lot of work, but great fun Bruce. And this all never would have come together without the contributions of so many here, esp. Dave Suponski, Jeff Kuss, and our friend the 'gold towel guy'.

No hay peor ciego que el que no quiere ver. None so blind as those who will not see.

Last edited by Drew Hause; 02-25-2016 at 06:15 PM..
Drew Hause is offline   Reply With Quote
The Following 4 Users Say Thank You to Drew Hause For Your Post:
Visit Drew Hause's homepage!
Unread 02-28-2016, 07:44 PM   #4
Member
Bruce Day
PGCA Lifetime
Member
 
Bruce Day's Avatar

Member Info
 
Join Date: Nov 2008
Posts: 4,995
Thanks: 554
Thanked 15,664 Times in 2,672 Posts

Default

Drew, several issues:

1. You identified an English steel maker named Titanic. Is this company the source of Parker Titanic barrels?

2. You identified several Krupp barrels. Lefever used Krupp barrels, but of which Krupp steel?

3. There has long been debate in the Parker community about whether Parker fluid steel grades were truly different or if the grade steels were the same and marketing was the difference. Your paper shows different compositions for Trojan, Vulcan, Parker Steel and Titanic. I think that settled that long standing question, agree ?
Bruce Day is offline   Reply With Quote
Unread 02-28-2016, 07:50 PM   #5
Member
Dean Romig
PGCA Invincible
Life Member
 
Dean Romig's Avatar

Member Info
 
Join Date: Dec 2008
Posts: 32,070
Thanks: 36,775
Thanked 34,208 Times in 12,646 Posts

Default

Quote:
Originally Posted by Bruce Day View Post
3. There has long been debate in the Parker community about whether Parker fluid steel grades were truly different or if the grade steels were the same and marketing was the difference. Your paper shows different compositions for Trojan, Vulcan, Parker Steel and Titanic. I think that settled that long standing question, agree ?

I think I'll read Dave's article again...

Seems to me there were some slight differences in a few of the steels Parker used.





.
__________________
"I'm a Setter man.
Not because I think they're better than the other breeds,
but because I'm a romantic - stuck on tradition - and to me, a Setter just "belongs" in the grouse picture."

George King, "That's Ruff", 2010 - a timeless classic.
Dean Romig is offline   Reply With Quote
Unread 02-28-2016, 07:59 PM   #6
Member
Drew Hause
Forum Associate
 
Drew Hause's Avatar

Member Info
 
Join Date: Nov 2008
Posts: 2,177
Thanks: 341
Thanked 3,998 Times in 1,309 Posts

Default

1. Robert Mushet's "Titanic Steel" was an early titanium alloy; different stuff.

2. Lefever and the other U.S. makers used Krupp Fluss Stahl but the composition may well have changed pre-1900 vs. pre-WWI.

3. Parker Steel = Acid Bessemer Resulphurized Rephosphorized AISI 1109 Carbon Steel. Somewhat similar to Parker Decarbonized or "Plain" Steel.

4. Titanic, post-WWI Vulcan, and Trojan were essentially the same; AISI 1030 and 1035 Medium Carbon steels.
Titanic did have low levels of both nickel and chromium compared to the others, but it would not be an "alloy steel".

5. Pre-1900 Vulcan was AISI 1015 with a lower tensile strength than AISI 1030.

We should however have pre-1900, pre-WWI, and post-WWI samples of each.

Last edited by Drew Hause; 02-28-2016 at 11:36 PM..
Drew Hause is offline   Reply With Quote
The Following 5 Users Say Thank You to Drew Hause For Your Post:
Visit Drew Hause's homepage!
Unread 05-25-2016, 01:50 PM   #7
Member
Richard Dow
PGCA Lifetime
Member

Member Info
 
Join Date: May 2009
Posts: 129
Thanks: 5
Thanked 102 Times in 47 Posts

Default

Drew: Thank you for your post.
Richard Dow is offline   Reply With Quote
The Following 7 Users Say Thank You to Richard Dow For Your Post:
Unread 06-09-2016, 05:34 PM   #8
Member
Drew Hause
Forum Associate
 
Drew Hause's Avatar

Member Info
 
Join Date: Nov 2008
Posts: 2,177
Thanks: 341
Thanked 3,998 Times in 1,309 Posts

Default

More interesting stuff on this Witten steel thread
http://www.doublegunshop.com/forums/...=445562&page=1

It is clear that even by 1880 the various steel producers were able to manufacture high carbon steel, and were working on the optimal manganese, and other alloy, concentrations. By 1890, Witten & Bofors were producing AISI 1044 which is good stuff.
Krupp was having problems getting enough manganese into their carbon steels at that point. Later Fluss Stahl was 1045 so they figured it out.
Whitworth was a medium carbon steel that also didn't quite have enough manganese to fit AISI criteria.
Drew Hause is offline   Reply With Quote
Visit Drew Hause's homepage!
Unread 06-14-2016, 07:20 PM   #9
Member
Drew Hause
Forum Associate
 
Drew Hause's Avatar

Member Info
 
Join Date: Nov 2008
Posts: 2,177
Thanks: 341
Thanked 3,998 Times in 1,309 Posts

Default

I've revised one of the documents to cover the evolution of iron & steel components in pattern welded barrels
https://docs.google.com/document/d/1...m8-_AQPiA/edit

I have a crolle and a twist barrel segment for composition analysis

Strength & composition of vintage new fangled steel barrels is still here
https://docs.google.com/document/d/1...EK8OtPYVA/edit
Drew Hause is offline   Reply With Quote
The Following 2 Users Say Thank You to Drew Hause For Your Post:
Visit Drew Hause's homepage!
Unread 08-11-2016, 03:48 PM   #10
Member
Drew Hause
Forum Associate
 
Drew Hause's Avatar

Member Info
 
Join Date: Nov 2008
Posts: 2,177
Thanks: 341
Thanked 3,998 Times in 1,309 Posts

Default

Just got the report from a Parker DD 6 Iron "Turkish" segment Dave graciously provided. The tensile strength was quite similar to other crolle specimens at 55,500 psi.
Composition analysis now of 3 crolle and 1 twist specimens confirms the steel component in crolle barrels was low carbon low alloy AISI 1002 – 1005.
Much more detailed articles will follow in DGJ.
Drew Hause is offline   Reply With Quote
The Following 4 Users Say Thank You to Drew Hause For Your Post:
Visit Drew Hause's homepage!
Reply


Posting Rules
You may not post new threads
You may not post replies
You may not post attachments
You may not edit your posts

BB code is On
Smilies are On
[IMG] code is On
HTML code is Off

Forum Jump


All times are GMT -4. The time now is 06:15 PM.

Powered by vBulletin® Version 3.8.4
Copyright ©2000 - 2024, Jelsoft Enterprises Ltd.
Copyright © 1998 - 2024, Parkerguns.org
Copyright © 2004 Design par Megatekno
- 2008 style update 3.7 avec l'autorisation de son auteur par Stradfred.